Menu
Property Feature Silicone Liner 60 Durometer Fluorosilicone Vamac Liner Viton Liner 500-FKM
Application Relevant Features *Less than 3% volume swell After 70 hrs In Boiling Coolant. *Less than 3% volume swell After 70 hrs In Boiling Coolant. *Less than 3% volume swell After 70 hrs In Boiling Coolant. *Less than 3% volume swell After 70 hrs In Boiling Coolant.
*Heat Resistant to 350⁰ F+. *Heat Resistance to 350⁰ F+ *Heat Resistant to 300⁰ F+ *Heat Resistance to 550⁰ F+
*1300 PSI Tensile. *1400 PSI Tensile. *2000 PSI Tensile *2400 PSI Tensile.
*Good Hot Tear  *Good Hot Tear *Low Hot Tear *Average Hot Tear.
*Will not pass Emission Control Specs, such as section 4 of TR 20521081, & SAE J 1527 (Hose Hydrocarbon barrier test) * Inadequate Permeation resistance (At same thickness as FKM liner) for SAE J1527, TR 20521081. Passes SAE J1527
ASTM #3 Oil, % VolumeChange After 7 Days at 300⁰ F +40 +5 +50 +4
Diesel Fuel, % Volume Change After 7 Days at 75⁰F +100 +17 +24 +1.5
Continuous Low Temperature use Down to 3⁰ F
Intermittent Temperature use -90⁰ F to + 550⁰ F -90⁰ F to + 550⁰ F From -41⁰ F to + 640⁰ F